Jataipeba vs Jatobá / jutaí-do-campo
Dialium guianense against Hymenaea parvifolia. Every number below names the publication it came from.
| Property | Jataipeba | Jatobá / jutaí-do-campo |
|---|---|---|
| Janka hardness | 3,650 lbfLPF/SFB Madeiras Brasileiras | 3,792 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 63.7 lb/ft³LPF/SFB Madeiras Brasileiras | 73.4 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 24,614 lb/in²LPF/SFB Madeiras Brasileiras | 24,635 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.35 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.46 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,481 lb/in²LPF/SFB Madeiras Brasileiras | 13,739 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 14.5%LPF/SFB Madeiras Brasileiras | 13.4%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.75LPF/SFB Madeiras Brasileiras | 2.62LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 4%. Choose on movement or on appearance instead.
- Jataipeba moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.6, so it is the safer choice for a wide flat panel.
- Jatobá / jutaí-do-campo is the heavier of the two by 156 kg/m³, which a reader building a door or a case should weigh.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.