Wood Record

Jatobá / jutaí-do-campo vs Marishballi

Hymenaea parvifolia against Lincania spp.. Every number below names the publication it came from.

PropertyJatobá / jutaí-do-campoMarishballi
Janka hardness3,792 lbfLPF/SFB Madeiras Brasileiras3,570 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC73.4 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-962.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture24,635 lb/in²LPF/SFB Madeiras Brasileiras27,700 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity2.46 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras3.34 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength13,739 lb/in²LPF/SFB Madeiras Brasileiras13,390 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)13.4%LPF/SFB Madeiras Brasileiras17.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)2.62LPF/SFB Madeiras Brasileiras1.56USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • Jatobá / jutaí-do-campo resists denting better. It tests 6% harder than Marishballi.
  • Marishballi moves more evenly. Its tangential-to-radial ratio is 1.6 against 2.6, so it is the safer choice for a wide flat panel.
  • Marishballi carries 12% more load in bending, which matters for a shelf or a rail.
  • Jatobá / jutaí-do-campo is the heavier of the two by 183 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons