PropertyKamassiTurpentine
Janka hardness2,730 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,750 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC58.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)60.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture20,970 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)19,700 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.54 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)2.23 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength10,530 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)11,400 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)——
Tangential / radial ratio(lower is better)——

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.