Kaneelhart vs Uxirana
Licaria spp. against Vantanea parviflora. Every number below names the publication it came from.
| Property | Kaneelhart | Uxirana |
|---|---|---|
| Janka hardness | 2,900 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2,948 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 69.7 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 29,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 24,635 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 4.06 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2.55 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 17,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 12,531 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 12.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 17.6%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.46USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.26LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 2%. Choose on movement or on appearance instead.
- Uxirana moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.5, so it is the safer choice for a wide flat panel.
- Kaneelhart carries 21% more load in bending, which matters for a shelf or a rail.
- Uxirana is the heavier of the two by 123 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.