Wood Record

Louro-faia vs Taniboca

Roupala montana against Buchenavia cf viridiflora. Every number below names the publication it came from.

PropertyLouro-faiaTaniboca
Janka hardness2,169 lbfLPF/SFB Madeiras Brasileiras2,191 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC61.3 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-954.9 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture22,957 lb/in²LPF/SFB Madeiras Brasileiras17,110 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.46 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras1.89 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength12,032 lb/in²LPF/SFB Madeiras Brasileiras9,587 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)18.0%LPF/SFB Madeiras Brasileiras11.2%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.95LPF/SFB Madeiras Brasileiras1.65LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Taniboca moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.0, so it is the safer choice for a wide flat panel.
  • Louro-faia carries 34% more load in bending, which matters for a shelf or a rail.
  • Louro-faia is the heavier of the two by 102 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons