Wood Record

Maçaranduba vs Mururé

Manilkara huberi against Brosimum gaudichaudii. Every number below names the publication it came from.

PropertyMaçarandubaMururé
Janka hardness3,047 lbfLPF/SFB Madeiras Brasileiras3,036 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC66.8 lb/ft³LPF/SFB Madeiras Brasileiras56.8 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture25,560 lb/in²LPF/SFB Madeiras Brasileiras19,941 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.47 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.06 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength15,774 lb/in²LPF/SFB Madeiras Brasileiras11,165 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)16.4%LPF/SFB Madeiras Brasileiras14.1%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.31LPF/SFB Madeiras Brasileiras1.82LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 0%. Choose on movement or on appearance instead.
  • Maçaranduba moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.8, so it is the safer choice for a wide flat panel.
  • Maçaranduba carries 28% more load in bending, which matters for a shelf or a rail.
  • Maçaranduba is the heavier of the two by 160 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons