Maçaranduba vs Pau-santo
Manilkara sp. against Zollernia paraensis. Every number below names the publication it came from.
| Property | Maçaranduba | Pau-santo |
|---|---|---|
| Janka hardness | 3,228 lbfLPF/SFB Madeiras Brasileiras | 3,261 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 66.8 lb/ft³LPF/SFB Madeiras Brasileiras | 78.7 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 24,593 lb/in²LPF/SFB Madeiras Brasileiras | 27,238 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.02 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.59 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 11,961 lb/in²LPF/SFB Madeiras Brasileiras | 13,854 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 16.4%LPF/SFB Madeiras Brasileiras | 16.8%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.40LPF/SFB Madeiras Brasileiras | 1.92LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Maçaranduba moves more evenly. Its tangential-to-radial ratio is 1.4 against 1.9, so it is the safer choice for a wide flat panel.
- Pau-santo carries 11% more load in bending, which matters for a shelf or a rail.
- Pau-santo is the heavier of the two by 190 kg/m³, which a reader building a door or a case should weigh.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.