Wood Record

Macawood vs Macucu-branco

Platymiscium spp. against Licania oblongifolia. Every number below names the publication it came from.

PropertyMacawoodMacucu-branco
Janka hardness3,150 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3,153 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC64.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)58.7 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture27,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b19,429 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity3.20 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.19 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength16,100 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b10,895 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)6.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-419.6%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.30USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.97LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 0%. Choose on movement or on appearance instead.
  • Macawood moves more evenly. Its tangential-to-radial ratio is 1.3 against 2.0, so it is the safer choice for a wide flat panel.
  • Macawood carries 42% more load in bending, which matters for a shelf or a rail.
  • Macawood is the heavier of the two by 85 kg/m³, which a reader building a door or a case should weigh.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons