Maria-preta vs Rosadinho
Zizyphus cinnamomum = Zizyphus itacaiunensis against Peltogyne paniculata. Every number below names the publication it came from.
| Property | Maria-preta | Rosadinho |
|---|---|---|
| Janka hardness | 3,331 lbfLPF/SFB Madeiras Brasileiras | 3,386 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 60.6 lb/ft³LPF/SFB Madeiras Brasileiras | 64.3 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 22,714 lb/in²LPF/SFB Madeiras Brasileiras | 27,138 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.35 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.57 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,688 lb/in²LPF/SFB Madeiras Brasileiras | 13,129 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 15.7%LPF/SFB Madeiras Brasileiras | 12.7%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.43LPF/SFB Madeiras Brasileiras | 1.59LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 2%. Choose on movement or on appearance instead.
- Rosadinho carries 19% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.