Wood Record

Marishballi vs Wamara

Lincania spp. against Swartzia spp.. Every number below names the publication it came from.

PropertyMarishballiWamara
Janka hardness3,570 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3,692 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture27,700 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b26,370 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity3.34 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3.63 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength13,390 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b15,440 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)17.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-411.2%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.56USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.95Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 3%. Choose on movement or on appearance instead.
  • Marishballi moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.9, so it is the safer choice for a wide flat panel.
  • Wamara is the heavier of the two by 128 kg/m³, which a reader building a door or a case should weigh.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.