Matamatá vs Urucurana

Eschweilera coriacea against Swartzia recurva. Every number below names the publication it came from.

PropertyMatamatáUrucurana
Janka hardness2,467 lbfLPF/SFB Madeiras Brasileiras2,469 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC56.2 lb/ft³LPF/SFB Madeiras Brasileiras57.4 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture19,002 lb/in²LPF/SFB Madeiras Brasileiras22,345 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.11 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.42 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength9,181 lb/in²LPF/SFB Madeiras Brasileiras10,596 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)16.0%LPF/SFB Madeiras Brasileiras15.0%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.71LPF/SFB Madeiras Brasileiras1.37LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 0%. Choose on movement or on appearance instead.
  • Urucurana moves more evenly. Its tangential-to-radial ratio is 1.4 against 1.7, so it is the safer choice for a wide flat panel.
  • Urucurana carries 18% more load in bending, which matters for a shelf or a rail.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.