Mecrusse vs Okan
Androstachys johnsonii against Cylicodiscus gabunensis. Every number below names the publication it came from.
| Property | Mecrusse | Okan |
|---|---|---|
| Janka hardness | 2,540 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,780 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 55.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 64.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 18,700 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 20,300 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | — | 2.33 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 9,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 12,380 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 11.6%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 12.6%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.07Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.47Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- Okan resists denting better. It tests 9% harder than Mecrusse.
- Mecrusse moves more evenly. Its tangential-to-radial ratio is 1.1 against 1.5, so it is the safer choice for a wide flat panel.
- Okan carries 9% more load in bending, which matters for a shelf or a rail.
- Okan is the heavier of the two by 146 kg/m³, which a reader building a door or a case should weigh.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.