Mecrusse vs Parinari / bafo-de-boi-mirim
Androstachys johnsonii against Parinari excelsa. Every number below names the publication it came from.
| Property | Mecrusse | Parinari / bafo-de-boi-mirim |
|---|---|---|
| Janka hardness | 2,540 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,522 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 55.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 57.4 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 18,700 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 21,164 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | — | 2.35 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 9,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 11,819 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 11.6%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 14.8%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.07Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.92LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Mecrusse moves more evenly. Its tangential-to-radial ratio is 1.1 against 1.9, so it is the safer choice for a wide flat panel.
- Parinari / bafo-de-boi-mirim carries 13% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.