Wood Record

Missanda vs Rhodesian-Teak

Erythrophleum ivorense against Baikiaea plurijuga. Every number below names the publication it came from.

PropertyMissandaRhodesian-Teak
Janka hardness2,930 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,990 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC56.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)56.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture23,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)12,220 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.24 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.23 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength14,100 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)9,600 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)——
Tangential / radial ratio(lower is better)——

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Missanda carries 92% more load in bending, which matters for a shelf or a rail.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.