Muirapixuna vs Rosadinho

Chamaecrista scleroxylon = Cassia scleroxylon against Peltogyne paniculata. Every number below names the publication it came from.

PropertyMuirapixunaRosadinho
Janka hardness3,435 lbfLPF/SFB Madeiras Brasileiras3,386 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC84.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-964.3 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture26,227 lb/in²LPF/SFB Madeiras Brasileiras27,138 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.38 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.57 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength13,967 lb/in²LPF/SFB Madeiras Brasileiras13,129 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)11.5%LPF/SFB Madeiras Brasileiras12.7%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)2.28LPF/SFB Madeiras Brasileiras1.59LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Rosadinho moves more evenly. Its tangential-to-radial ratio is 1.6 against 2.3, so it is the safer choice for a wide flat panel.
  • Muirapixuna is the heavier of the two by 317 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.