Wood Record

Oak vs Pau-branco

Quercus spp. against Drypetes variabilis. Every number below names the publication it came from.

PropertyOakPau-branco
Janka hardness2,500 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2,518 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)55.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture23,000 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b20,865 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity3.02 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.30 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength2,960 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)10,511 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)18.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-415.9%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.83USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.95LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Oak carries 10% more load in bending, which matters for a shelf or a rail.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons