Wood Record

Sucupira vs Tanimbuca

Bowdichia nitida against Buchenavia sp. Every number below names the publication it came from.

PropertySucupiraTanimbuca
Janka hardness2,903 lbfLPF/SFB Madeiras Brasileiras2,829 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC59.9 lb/ft³LPF/SFB Madeiras Brasileiras53.7 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture23,663 lb/in²LPF/SFB Madeiras Brasileiras19,756 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.33 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.03 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength13,536 lb/in²LPF/SFB Madeiras Brasileiras10,582 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)12.3%LPF/SFB Madeiras Brasileiras12.7%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.64LPF/SFB Madeiras Brasileiras1.89LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 3%. Choose on movement or on appearance instead.
  • Sucupira moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.9, so it is the safer choice for a wide flat panel.
  • Sucupira carries 20% more load in bending, which matters for a shelf or a rail.
  • Sucupira is the heavier of the two by 100 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons