| Property | Tanimbuca | Tanimbuca |
|---|---|---|
| Janka hardness | 2,829 lbfLPF/SFB Madeiras Brasileiras | 2,235 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 53.7 lb/ft³LPF/SFB Madeiras Brasileiras | 64.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 19,756 lb/in²LPF/SFB Madeiras Brasileiras | 21,178 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.03 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.03 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 10,582 lb/in²LPF/SFB Madeiras Brasileiras | 11,307 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 12.7%LPF/SFB Madeiras Brasileiras | 12.8%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.89LPF/SFB Madeiras Brasileiras | 1.50LPF/SFB Madeiras Brasileiras |
What the numbers mean
- Tanimbuca resists denting better. It tests 27% harder than Tanimbuca.
- Tanimbuca moves more evenly. Its tangential-to-radial ratio is 1.5 against 1.9, so it is the safer choice for a wide flat panel.
- Tanimbuca is the heavier of the two by 167 kg/m³, which a reader building a door or a case should weigh.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain