The family Fagaceae supplies 84 of the timbers in this database. A family shares broad anatomy, but not necessarily working properties.
21 of 84 carry a published Janka test.
| Wood | Janka | Density |
|---|---|---|
| Allegheny chinkapinCastanea pumila | 573 lbf* | 29.8 lb/ft³ |
| American beechFagus grandifolia | 1,300 lbf | 44.8 lb/ft³ |
| American chestnutCastanea dentata | 540 lbf | 30.1 lb/ft³ |
| Arizona white oakQuercus arizonica | 1,419 lbf* | 45.5 lb/ft³ |
| Arkansas oakQuercus arkansana | 1,419 lbf* | 45.5 lb/ft³ |
| Bastard oakQuercus sinuata | 1,475 lbf* | 46.4 lb/ft³ |
| Bastard white oakQuercus austrina | 2,210 lbf* | 55.9 lb/ft³ |
| BeranganCastanopsis spp. | 960 lbf* | 42.0 lb/ft³ |
| Black oakQuercus velutina | 1,210 lbf | 42.6 lb/ft³ |
| Blackjack oakQuercus marilandica | 1,419 lbf* | 45.5 lb/ft³ |
| Blue oakQuercus douglasii | 1,419 lbf* | 45.5 lb/ft³ |
| Bluejack oakQuercus incana | 1,419 lbf* | 45.5 lb/ft³ |
| Buckley oakQuercus buckleyi | 1,419 lbf* | 45.5 lb/ft³ |
| Bur oakQuercus macrocarpa | 1,370 lbf | 44.8 lb/ft³ |
| California black oakQuercus kelloggii | 1,007 lbf* | 38.8 lb/ft³ |
| California live oakQuercus agrifolia | 1,419 lbf* | 45.5 lb/ft³ |
| California white oakQuercus lobata | 1,203 lbf* | 42.1 lb/ft³ |
| Canyon live oakQuercus chrysolepis | 2,139 lbf* | 55.1 lb/ft³ |
| Cherrybark oakQuercus pagoda | 1,480 lbf | 47.6 lb/ft³ |
| Chestnut oakQuercus prinus | 1,130 lbf | 46.1 lb/ft³ |
| Chinese chestnutCastanea mollissima | 573 lbf* | 29.8 lb/ft³ |
| Chinkapin oakQuercus muehlenbergii | 1,419 lbf* | 45.5 lb/ft³ |
| Chisos oakQuercus graciliformis | 1,419 lbf* | 45.5 lb/ft³ |
| Cork oakQuercus suber | 2,287 lbf* | 56.9 lb/ft³ |
| Darlington oakQuercus hemisphaerica | 1,419 lbf* | 45.5 lb/ft³ |
| Delta post oakQuercus similis | 1,419 lbf* | 45.5 lb/ft³ |
| Durmast oakQuercus petraea | 1,419 lbf* | 45.5 lb/ft³ |
| Dwarf chinkapin oakQuercus prinoides | 1,419 lbf* | 45.5 lb/ft³ |
| Dwarf live oakQuercus minima | 1,419 lbf* | 45.5 lb/ft³ |
| Dwarf post oakQuercus margarettiae | 1,419 lbf* | 45.5 lb/ft³ |
| Emory oakQuercus emoryi | 1,419 lbf* | 45.5 lb/ft³ |
| Engelmann oakQuercus engelmannii | 1,419 lbf* | 45.5 lb/ft³ |
| European beechFagus sylvatica | 1,054 lbf* | 39.6 lb/ft³ |
| European oakQuercus robur | 1,309 lbf* | 43.8 lb/ft³ |
| European turkey oakQuercus cerris | 1,419 lbf* | 45.5 lb/ft³ |
| Gambel oakQuercus gambelii | 1,538 lbf* | 47.3 lb/ft³ |
| Graves oakQuercus gravesii | 1,419 lbf* | 45.5 lb/ft³ |
| Gray oakQuercus grisea | 1,419 lbf* | 45.5 lb/ft³ |
| Havard oakQuercus havardii | 1,419 lbf* | 45.5 lb/ft³ |
| Holly oakQuercus ilex | 1,419 lbf* | 45.5 lb/ft³ |
| Interior live oakQuercus wislizeni | 1,419 lbf* | 45.5 lb/ft³ |
| Japanese chestnutCastanea crenata | 573 lbf* | 29.8 lb/ft³ |
| Lacey oakQuercus laceyi | 1,419 lbf* | 45.5 lb/ft³ |
| Lateleaf oakQuercus tardifolia | 1,419 lbf* | 45.5 lb/ft³ |
| Laurel oakQuercus laurifolia | 1,210 lbf | 44.1 lb/ft³ |
| Live oakQuercus virginiana | 2,712 lbf* | 61.6 lb/ft³ |
| Mexican blue oakQuercus oblongifolia | 1,419 lbf* | 45.5 lb/ft³ |
| Mexican white oakQuercus polymorpha | 1,419 lbf* | 45.5 lb/ft³ |
| Myrtle oakQuercus myrtifolia | 1,419 lbf* | 45.5 lb/ft³ |
| Netleaf oakQuercus rugosa | 1,419 lbf* | 45.5 lb/ft³ |
| Northern pin oakQuercus ellipsoidalis | 1,419 lbf* | 45.5 lb/ft³ |
| Northern red oakQuercus rubra | 1,290 lbf | 44.1 lb/ft³ |
| Nuttall oakQuercus texana | 1,419 lbf* | 45.5 lb/ft³ |
| OakQuercus spp. | 2,500 lbf | 53.0 lb/ft³ |
| Oglethorpe oakQuercus oglethorpensis | 1,419 lbf* | 45.5 lb/ft³ |
| Oregon white oakQuercus garryana | 1,725 lbf* | 49.9 lb/ft³ |
| Overcup oakQuercus lyrata | 1,190 lbf | 44.1 lb/ft³ |
| Pin oakQuercus palustris | 1,510 lbf | 44.1 lb/ft³ |
| Post oakQuercus stellata | 1,360 lbf | 46.8 lb/ft³ |
| Pungent oakQuercus pungens | 1,419 lbf* | 45.5 lb/ft³ |
| RauliNothofagus spp. | 990 lbf | 37.1 lb/ft³ |
| Robust oakQuercus robusta | 1,419 lbf* | 45.5 lb/ft³ |
| Sand live oakQuercus geminata | 1,419 lbf* | 45.5 lb/ft³ |
| Sandpaper oakQuercus vaseyana | 1,419 lbf* | 45.5 lb/ft³ |
| Sawtooth oakQuercus acutissima | 1,419 lbf* | 45.5 lb/ft³ |
| Scarlet oakQuercus coccinea | 1,400 lbf | 46.8 lb/ft³ |
| Scrub oakQuercus ilicifolia | 1,419 lbf* | 45.5 lb/ft³ |
| Shingle oakQuercus imbricaria | 1,419 lbf* | 45.5 lb/ft³ |
| Shumard oakQuercus shumardii | 1,419 lbf* | 45.5 lb/ft³ |
| Silverleaf oakQuercus hypoleucoides | 1,419 lbf* | 45.5 lb/ft³ |
| Sonoran scrub oakQuercus turbinella | 1,419 lbf* | 45.5 lb/ft³ |
| Southern red oakQuercus falcata | 1,060 lbf | 41.3 lb/ft³ |
| Swamp chestnut oakQuercus michauxii | 1,240 lbf | 46.8 lb/ft³ |
| Swamp white oakQuercus bicolor | 1,620 lbf | 50.3 lb/ft³ |
| Sweet chestnutCastanea sativa | 1,103 lbf* | 40.5 lb/ft³ |
| TanoakNotholithocarpus densiflorus | 1,363 lbf* | 44.7 lb/ft³ |
| TanoakLithocarpus densiflorus | 1,363 lbf* | 44.7 lb/ft³ |
| Tasmanian-MyrtleNothofagus spp. | 1,325 lbf | 39.0 lb/ft³ |
| Texas live oakQuercus fusiformis | 1,475 lbf* | 46.4 lb/ft³ |
| Toumey oakQuercus toumeyi | 1,419 lbf* | 45.5 lb/ft³ |
| Turkey oakQuercus laevis | 1,419 lbf* | 45.5 lb/ft³ |
| Water oakQuercus nigra | 1,190 lbf | 44.1 lb/ft³ |
| White oakQuercus alba | 1,360 lbf | 47.6 lb/ft³ |
| Willow oakQuercus phellos | 1,460 lbf | 48.3 lb/ft³ |