family
Lauraceae
The family Lauraceae supplies 47 of the timbers in this database. A family shares broad anatomy, but not necessarily working properties.
24 of 47 carry a published Janka test.
| Wood | Janka | Density |
|---|---|---|
| AbacatiranaOcotea aciphylla = Ocotea costulata | 1,025 lbf | 38.7 lb/ft³ |
| AvocadoPersea americana | 791 lbf* | 34.7 lb/ft³ |
| BelianEusideroxylon zwageri | 3,020 lbf | 68.0 lb/ft³ |
| California laurelUmbellularia californica | 1,007 lbf* | 38.8 lb/ft³ |
| CamphortreeCinnamomum camphora | 875 lbf* | 36.3 lb/ft³ |
| Canela/louro-tamancoNectandra cuspidata | 573 lbf* | 28.7 lb/ft³ |
| CanelilloAniba bracteata | 1,419 lbf* | 45.5 lb/ft³ |
| CaneloNectandra spp. | 1,060 lbf | 39.0 lb/ft³ |
| Casca-preciosaAniba canelilla | 3,369 lbf | 75.4 lb/ft³ |
| CassiaCinnamomum aromaticum | 915 lbf* | 37.1 lb/ft³ |
| CinnamonCinnamomum verum | 1,054 lbf* | 39.6 lb/ft³ |
| Cinnamon WoodCinnamomum spp. | 660 lbf* | 32.0 lb/ft³ |
| Demerara GreenheartOcotea rodiaei | 2,360 lbf | 66.0 lb/ft³ |
| DetermaOcotea rubra | 660 lbf | 42.0 lb/ft³ |
| East African CamphorwoodOcotea usambarensis | 930 lbf | 37.0 lb/ft³ |
| GreenheartChlorocardium rodiei | 2,350 lbf | 64.1 lb/ft³ |
| HolioCryptocarya mannii | 1,007 lbf* | 38.8 lb/ft³ |
| ImbuiaPhoebe porosa | 950 lbf | 40.0 lb/ft³ |
| ItaúbaMezilaurus lindaviana | 992 lbf | 53.3 lb/ft³ |
| Itaúba / itaúba-vermelhaMezilaurus itauba | 1,262 lbf | 54.2 lb/ft³ |
| KaneelhartLicaria spp. | 2,900 lbf | 62.0 lb/ft³ |
| Laurel espadaOcotea floribunda | 753 lbf* | 33.9 lb/ft³ |
| LinguePersea spp. | 860 lbf | 36.0 lb/ft³ |
| Loblolly sweetwoodOcotea leucoxylon | 915 lbf* | 37.1 lb/ft³ |
| LouroOcotea sp. | 1,198 lbf | 38.4 lb/ft³ |
| LouroAnaueria brasiliensis = Beilschmiedia brasiliensis | 1,257 lbf | 45.6 lb/ft³ |
| Louro-amareloLicaria chrysophylla = Licaria rigida | 2,019 lbf | 57.7 lb/ft³ |
| Louro-mamorimOcotea cymbarum = Ocotea barcellensis | 1,135 lbf | 42.1 lb/ft³ |
| Louro-pretoOcotea neesiana | 1,010 lbf | 42.1 lb/ft³ |
| Louro-pretoOcotea fragrantissima | 1,063 lbf | 36.2 lb/ft³ |
| Louro-vermelhoSextonia rubra = Nectandra rubra | 756 lbf | 42.1 lb/ft³ |
| MachilusMachilus spp. | 630 lbf | 32.0 lb/ft³ |
| MedangLitsea spp. | 562 lbf | 31.0 lb/ft³ |
| Nectandra membranaceaNectandra membranacea | 875 lbf* | 36.3 lb/ft³ |
| Nectandra turbacensisNectandra turbacensis | 1,103 lbf* | 40.5 lb/ft³ |
| NemocaOcotea moschata | 1,419 lbf* | 45.5 lb/ft³ |
| Nemoca cimarronaOcotea spathulata | 1,419 lbf* | 45.5 lb/ft³ |
| OrientalwoodEndiandra palmerstonii | 1,203 lbf* | 42.0 lb/ft³ |
| Pepperleaf sweetwoodLicaria triandra | 1,923 lbf* | 52.4 lb/ft³ |
| Puerto Rico cinnamonLicaria parvifolia | 2,367 lbf* | 57.7 lb/ft³ |
| RedbayPersea borbonia | 1,007 lbf* | 38.8 lb/ft³ |
| Rose-MapieCryptocarya spp. | 1,515 lbf | 45.0 lb/ft³ |
| SassafrasSassafras albidum | 672 lbf* | 32.2 lb/ft³ |
| ShinglewoodNectandra hihua | 679 lbf* | 32.3 lb/ft³ |
| SlugwoodBeilschmiedia pendula | 1,255 lbf* | 43.0 lb/ft³ |
| Swamp bayPersea palustris | 1,152 lbf* | 41.3 lb/ft³ |
| TawaBeilschmiedia tawa | 1,405 lbf | 44.0 lb/ft³ |