Rhamnaceae
The family Rhamnaceae supplies 12 of the timbers in this database. A family shares broad anatomy, but not necessarily working properties.
2 of 12 carry a published Janka test.
| Wood | Janka | Density |
|---|---|---|
| BluewoodCondalia hookeri | 3,860 lbf* | 72.5 lb/ft³ |
| California buckthornFrangula californica | 960 lbf* | 38.0 lb/ft³ |
| Common buckthornRhamnus cathartica | 1,725 lbf* | 49.9 lb/ft³ |
| Greenheart, common snakebarkColubrina arborescens | 1,725 lbf* | 49.9 lb/ft³ |
| Indian jujubeZiziphus mauritiana | 1,419 lbf* | 45.5 lb/ft³ |
| Japanese raisintreeHovenia dulcis | 1,203 lbf* | 42.1 lb/ft³ |
| LeadwoodKrugiodendron ferreum | 4,921 lbf* | 81.2 lb/ft³ |
| Maria-pretaZizyphus cinnamomum = Zizyphus itacaiunensis | 3,331 lbf | 60.6 lb/ft³ |
| MusiziMaesopsis eminii | 600 lbf | 30.0 lb/ft³ |
| Pink ivoryBerchemia zeyheri | 2,963 lbf* | 64.1 lb/ft³ |
| SoldierwoodColubrina elliptica | 2,367 lbf* | 57.7 lb/ft³ |
| ToiAlphitonia zizyphoides | 960 lbf* | 38.0 lb/ft³ |