The family Sapotaceae supplies 52 of the timbers in this database. A family shares broad anatomy, but not necessarily working properties.

25 of 52 carry a published Janka test.

WoodJankaDensity
Abiu-brancoPouteria oppositifolia1,788 lbf*50.7 lb/ft³
AbiuranaPouteria anomala2,472 lbf56.2 lb/ft³
AbiuranaPouteria sp2,418 lbf57.4 lb/ft³
AbiuranaPouteria egregia2,950 lbf67.7 lb/ft³
AbiuranaPouteria guianensis2,921 lbf58.7 lb/ft³
Abiurana-brancaPouteria caimito2,608 lbf56.8 lb/ft³
Abiurana-brancaMicropholis mensalis1,605 lbf46.2 lb/ft³
Abiurana-mangabaranaMicropholis guyanensis1,781 lbf48.7 lb/ft³
Abiurana-secaDiploon cuspidatum = Diploon venezuelana2,945 lbf68.7 lb/ft³
AningeriaAningeria spp.995 lbf33.0 lb/ft³
Bastard redwoodChrysophyllum argenteum2,692 lbf*61.3 lb/ft³
BreakbillSideroxylon obovatum2,287 lbf*56.9 lb/ft³
Buckthorn bullySideroxylon lycioides1,054 lbf*39.6 lb/ft³
BulletwoodManilkara bidentata3,190 lbf66.0 lb/ft³
Bulletwood, elengiMimusops elengi2,867 lbf*63.1 lb/ft³
BullytreePouteria multiflora2,064 lbf*54.2 lb/ft³
Caimitillo verdeMicropholis garciniifolia1,923 lbf*52.4 lb/ft³
CaimitoCynodendron spp-2,530 lbf*59.6 lb/ft³
ChupónPradosia spp.1,880 lbf52.0 lb/ft³
EggfruitPouteria campechiana2,448 lbf*58.7 lb/ft³
False masticSideroxylon foetidissimum3,241 lbf*66.9 lb/ft³
GasuPalaquium stehlinii1,007 lbf*38.8 lb/ft³
GoiabãoChrysophyllum lucentifolium = Pouteria pachycarpa2,646 lbf58.1 lb/ft³
GrumixavaMicropholis spp.1,490 lbf46.0 lb/ft³
LalahagPlanchonella obovata1,990 lbf*53.3 lb/ft³
LonguiGambeya africana1,658 lbf*48.9 lb/ft³
MaçarandubaManilkara sp.3,228 lbf66.8 lb/ft³
MaçarandubaManilkara huberi3,047 lbf66.8 lb/ft³
MaçarandubaranaChrysophyllum prieurii2,725 lbf61.8 lb/ft³
MakoréTieghemella heckelii1,110 lbf42.0 lb/ft³
MamalavaPlanchonella torricellensis1,363 lbf*44.7 lb/ft³
Mammee sapotePouteria sapota1,923 lbf*52.4 lb/ft³
MaragonçaloPouteria obscura1,746 lbf48.7 lb/ft³
MoabiBaillonella toxisperma2,210 lbf*55.0 lb/ft³
MukulunguAutranella congolensis2,779 lbf*60.0 lb/ft³
NyatohPalaquium spp.1,018 lbf42.0 lb/ft³
PaniManilkara dissecta3,749 lbf*71.5 lb/ft³
Puerto Rico bullySideroxylon portoricense2,692 lbf*61.3 lb/ft³
RosadinhoMicropholis venulosa1,720 lbf52.4 lb/ft³
RosadinhoPeltogyne paniculata3,386 lbf64.3 lb/ft³
RosadinhoPiptadenia gonoacantha = Piptadenia communis1,669 lbf53.3 lb/ft³
Saffron plumSideroxylon celastrinum1,923 lbf*52.4 lb/ft³
SapodillaManilkara zapota3,054 lbf*65.0 lb/ft³
SatinleafChrysophyllum oliviforme2,607 lbf*60.4 lb/ft³
SorvaMalouetia duckei1,329 lbf43.8 lb/ft³
Star appleChrysophyllum cainito2,448 lbf*58.7 lb/ft³
Tamaulipan ComaSideroxylon laetevirens1,054 lbf*39.6 lb/ft³
Tough bullySideroxylon tenax1,054 lbf*39.6 lb/ft³
TuturubáPouteria gongrijpii = Franchetella gongrijpii2,396 lbf56.9 lb/ft³
TuturubáPouteria oblanceolata2,923 lbf59.9 lb/ft³
Wild dillyManilkara jaimiqui3,147 lbf*65.9 lb/ft³
Willow busticSideroxylon salicifolium2,867 lbf*63.1 lb/ft³