Wood Record

Brush Box vs Turpentine

Tristania spp. against Syncarpia glomulifera. Every number below names the publication it came from.

PropertyBrush BoxTurpentine
Janka hardness3,088 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,750 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)60.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture26,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)19,700 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.68 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)2.23 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength11,700 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)11,400 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)——
Tangential / radial ratio(lower is better)1.90Chudnoff 1984, Tropical Timbers of the World (AH-607)—

What the numbers mean

  • Brush Box resists denting better. It tests 12% harder than Turpentine.
  • Brush Box carries 33% more load in bending, which matters for a shelf or a rail.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons