Sucupira vs Sucupira
Bowdichia nitida against Diplotropis purpurea. Every number below names the publication it came from.
| Property | Sucupira | Sucupira |
|---|---|---|
| Janka hardness | 2,903 lbfLPF/SFB Madeiras Brasileiras | 2,140 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 59.9 lb/ft³LPF/SFB Madeiras Brasileiras | 56.2 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 23,663 lb/in²LPF/SFB Madeiras Brasileiras | 20,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.33 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.87 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 13,536 lb/in²LPF/SFB Madeiras Brasileiras | 12,140 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | 12.3%LPF/SFB Madeiras Brasileiras | 11.8%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.64LPF/SFB Madeiras Brasileiras | 1.52USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- Sucupira resists denting better. It tests 36% harder than Sucupira.
- Sucupira carries 15% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.