Cupressaceae
The family Cupressaceae supplies 38 of the timbers in this database. A family shares broad anatomy, but not necessarily working properties.
12 of 38 carry a published Janka test.
| Wood | Janka | Density |
|---|---|---|
| African Pencil CedarJuniperus procera | 717 lbf* | 36.0 lb/ft³ |
| AlerceFitzroya cupressoides | 560 lbf | 30.0 lb/ft³ |
| Alligator juniperJuniperus deppeana | 717 lbf* | 36.3 lb/ft³ |
| Ashe juniperJuniperus ashei | 645 lbf* | 33.9 lb/ft³ |
| Atlantic white cedarChamaecyparis thyoides | 350 lbf | 22.3 lb/ft³ |
| BaldcypressTaxodium distichum | 510 lbf | 32.2 lb/ft³ |
| Bermuda juniperJuniperus bermudiana | 792 lbf* | 38.8 lb/ft³ |
| California juniperJuniperus californica | 645 lbf* | 33.9 lb/ft³ |
| Callitris columellarisCallitris columellaris | 926 lbf* | 43.0 lb/ft³ |
| Chinese firCunninghamia lanceolata | 390 lbf* | 24.3 lb/ft³ |
| Chinese juniperJuniperus chinensis | 645 lbf* | 33.9 lb/ft³ |
| Dawn redwoodMetasequoia glyptostroboides | 371 lbf* | 23.5 lb/ft³ |
| Drooping juniperJuniperus flaccida | 645 lbf* | 33.9 lb/ft³ |
| Eastern redcedarJuniperus virginiana | 615 lbf* | 32.8 lb/ft³ |
| Giant sequoiaSequoiadendron giganteum | 408 lbf* | 25.1 lb/ft³ |
| HinokiChamaecyparis obtusa | 599 lbf* | 32.3 lb/ft³ |
| Incense cedarCalocedrus decurrens | 470 lbf | 25.8 lb/ft³ |
| Italian cypressCupressus sempervirens | 740 lbf* | 37.1 lb/ft³ |
| Japanese cedarCryptomeria japonica | 371 lbf* | 23.5 lb/ft³ |
| Mexican cypressCupressus lustianica | 460 lbf | 32.0 lb/ft³ |
| Mlanje-CedarWiddringtonia whytei | 645 lbf* | 34.0 lb/ft³ |
| Montezuma baldcypressTaxodium mucronatum | 576 lbf* | 31.5 lb/ft³ |
| Northern white cedarThuja occidentalis | 320 lbf | 21.7 lb/ft³ |
| Old-growth redwoodSequoia sempervirens | 480 lbf | 28.0 lb/ft³ |
| Oneseed juniperJuniperus monosperma | 645 lbf* | 33.9 lb/ft³ |
| Oriental arborvitaePlatycladus orientalis | 818 lbf* | 39.6 lb/ft³ |
| Pinchot juniperJuniperus pinchotii | 645 lbf* | 33.9 lb/ft³ |
| PondcypressTaxodium ascendens | 576 lbf* | 31.5 lb/ft³ |
| Port-Orford cedarChamaecyparis lawsoniana | 630 lbf | 30.1 lb/ft³ |
| Redberry juniperJuniperus coahuilensis | 645 lbf* | 33.9 lb/ft³ |
| Rocky Mountain juniperJuniperus scopulorum | 645 lbf* | 33.9 lb/ft³ |
| Sawara-cypressChamaecyparis pisifera | 469 lbf* | 27.5 lb/ft³ |
| Utah juniperJuniperus osteosperma | 1,282 lbf* | 53.3 lb/ft³ |
| Western juniperJuniperus occidentalis | 645 lbf* | 33.9 lb/ft³ |
| Western redcedarThuja plicata | 350 lbf | 22.3 lb/ft³ |
| White Cypress-PineCallitris glauca | 1,375 lbf | 42.0 lb/ft³ |
| Yellow cedarChamaecyparis nootkatensis | 580 lbf | 30.8 lb/ft³ |
| Young-growth redwoodSequoia sempervirens | 420 lbf | 24.5 lb/ft³ |