Best wood for decking
Choose a complete deck system, including suitable boards, spacing, and fasteners.

Which wood should you choose?
Ipe is a candidate for a dense, wear-resistant hardwood deck. Properly specified pressure-treated lumber is a practical budget option, and western red cedar suits projects prioritizing low weight and easier machining. The best deck board depends on exposure, maintenance, local supply, and the supporting structure.
Practical wood choices
These editorial choices account for the application as well as the numbers. They may differ from the automated property ranking below.
Ipe
Very dense and hard-wearing, with demanding cutting and fastening. Budget for predrilling, appropriate tooling, and the weight of the material. Confirm species, sourcing, and the supplier's installation requirements.
Species profiles:Ipe
Pressure-treated lumber
Often the economical choice when the treatment and product rating match the exposure. It is a treated product rather than a single species; moisture condition and installation guidance matter as much as the species name.
Western red cedar
Easier to cut and handle than dense tropical hardwoods. Expect a softer walking surface and check the grade and heartwood content. Board thickness and support spacing must follow the product and design requirements.
Species profiles:Western redcedar
What matters for this project
Hardness helps compare dent resistance, while bending properties describe a different aspect of performance. Neither provides an approved joist spacing. Decay resistance, treatment, surface traction, splintering, and fastener compatibility are separate decisions. Compare complete installed cost rather than the price of a single board.
What to check before you buy
Check actual board dimensions, grade, moisture condition, and available lengths before planning the layout. Ask which fasteners and end treatment the supplier specifies. Order enough allowance for defects and trimming without assuming that an expensive board is automatically clear or straight.
Building and looking after it
Follow the decking manufacturer's spacing and fastening instructions for the wood's moisture condition. Maintain ventilation and drainage, and protect vulnerable end grain as directed. Dense boards commonly need predrilling. Inspect the finished surface and fasteners periodically, especially near steps, edges, and areas that stay wet.
Mistakes to avoid
Do not use this table's clear-wood strength values as structural design values. It also does not assess preservative treatment, decay durability, or slip resistance. The deck frame, connections, and board spans need their own suitable specification.
Property comparison ranking
Bending strength at least 12,000 psi. The score combines Janka hardness divided by 4,000 and bending strength divided by 30,000.
This score does not assess decay resistance, slip resistance, material grade, span, connections, or allowable design loads. Hardness and clear-wood bending strength alone do not establish suitability for a deck.
Species enter when the required fields are present and the rule gives a positive score. An absent wood may lack data or fall outside the scoring range; absence is not proof that it is unsuitable.
The order also uses an editorial availability multiplier, shown in the last column. It changes the order without removing a qualifying species. These scores compare selected properties; they do not evaluate every requirement of the finished project.
| # | Wood | Janka | Density | MOR | MOE | Shrinkage | T/R | Availability |
|---|---|---|---|---|---|---|---|---|
| 1 | Ipe | 3,680 lbf | 70.0 lb/ft³ | 25,400 lb/in² | 3.14 ×10⁶ lb/in² | 13.2% | 1.21 | |
| 2 | Cumaru | 3,415 lbf | 66.8 lb/ft³ | 24,371 lb/in² | 2.43 ×10⁶ lb/in² | 13.5% | 1.56 | |
| 3 | Bubinga | 2,690 lbf | 55.9 lb/ft³ | 22,600 lb/in² | 2.48 ×10⁶ lb/in² | 14.2% | 1.45 | |
| 4 | Indian rosewood | 3,170 lbf | 53.0 lb/ft³ | 16,900 lb/in² | 1.78 ×10⁶ lb/in² | 8.5% | 2.15 | |
| 5 | Marishballi | 3,570 lbf | 62.0 lb/ft³ | 27,700 lb/in² | 3.34 ×10⁶ lb/in² | 17.2% | 1.56 | |
| 6 | Azobe | 3,350 lbf | 70.0 lb/ft³ | 24,500 lb/in² | 2.47 ×10⁶ lb/in² | 17.0% | 1.31 | |
| 7 | Shagbark hickory | 1,880 lbf | 50.3 lb/ft³ | 20,200 lb/in² | 2.16 ×10⁶ lb/in² | 16.7% | 1.50 | |
| 8 | Mockernut hickory | 1,970 lbf | 50.3 lb/ft³ | 19,200 lb/in² | 2.22 ×10⁶ lb/in² | 17.8% | 1.43 | |
| 9 | Purpleheart | 1,860 lbf | 58.0 lb/ft³ | 19,200 lb/in² | 2.27 ×10⁶ lb/in² | 9.9% | 1.91 | |
| 10 | East African Olive | 2,740 lbf | 55.0 lb/ft³ | 25,300 lb/in² | 2.53 ×10⁶ lb/in² | — | — | |
| 11 | African ebony | 3,220 lbf | 63.0 lb/ft³ | 21,200 lb/in² | — | 20.0% | 1.17 | |
| 12 | Greenheart | 2,350 lbf | 64.1 lb/ft³ | 24,900 lb/in² | 3.25 ×10⁶ lb/in² | 17.1% | 1.09 | |
| 13 | Jarrah | 1,910 lbf | 54.0 lb/ft³ | 16,200 lb/in² | 1.88 ×10⁶ lb/in² | 18.7% | 1.43 | |
| 14 | Kamassi | 2,730 lbf | 58.0 lb/ft³ | 20,970 lb/in² | 2.54 ×10⁶ lb/in² | — | — | |
| 15 | Keruing | 1,270 lbf | 54.2 lb/ft³ | 19,900 lb/in² | 2.07 ×10⁶ lb/in² | 16.1% | 2.10 | |
| 16 | Cherrybark oak | 1,480 lbf | 47.6 lb/ft³ | 18,100 lb/in² | 2.28 ×10⁶ lb/in² | — | — | |
| 17 | Panga Panga | 1,630 lbf | 55.0 lb/ft³ | 16,200 lb/in² | 1.97 ×10⁶ lb/in² | — | 1.87 | |
| 18 | Brazilian rosewood | 2,720 lbf | 64.1 lb/ft³ | 19,000 lb/in² | 1.88 ×10⁶ lb/in² | 8.5% | 1.59 | |
| 19 | Ramin | 1,300 lbf | 39.6 lb/ft³ | 18,500 lb/in² | 2.17 ×10⁶ lb/in² | 13.4% | 2.02 | |
| 20 | Bitternut hickory | 1,461 lbf* | 46.1 lb/ft³ | 17,100 lb/in² | 1.79 ×10⁶ lb/in² | — | — | |
| 21 | Merbau | 1,500 lbf | 50.0 lb/ft³ | 16,800 lb/in² | 2.23 ×10⁶ lb/in² | 7.8% | 1.70 | |
| 22 | Sweet birch | 1,470 lbf | 45.4 lb/ft³ | 16,900 lb/in² | 2.17 ×10⁶ lb/in² | 15.6% | 1.38 | |
| 23 | Pecan hickory | 1,820 lbf | 46.1 lb/ft³ | 13,700 lb/in² | 1.73 ×10⁶ lb/in² | 13.6% | 1.82 | |
| 24 | Sucupira | 2,448 lbf* | 58.7 lb/ft³ | 19,400 lb/in² | — | 13.4% | 1.56 | |
| 25 | Sugar maple | 1,450 lbf | 44.1 lb/ft³ | 15,800 lb/in² | 1.83 ×10⁶ lb/in² | 14.7% | 2.06 |
Before you choose a board
Use this ranking to compare the properties listed above. Grain direction, defects, moisture content, board dimensions, and construction also affect performance. Check the species page for the original measurements and any estimate marks, then inspect the actual stock you can buy.
The score does not assess decay resistance, food-contact suitability, heat resistance, or structural load capacity. For outdoor work, check durability and treatment requirements separately. For food-contact items and toys, check the intended finish and published safety information.
Read wood allergy and toxicity sourcesHow to read the measurements
Janka compares resistance to indentation. Density is the mass of a given volume of wood. Modulus of rupture (MOR) describes bending strength in a test specimen. Shrinkage figures describe the change from green to oven-dry wood, and T/R compares tangential with radial shrinkage. They are useful for comparison, but do not directly predict seasonal movement in your finished piece.
These are species-level reference values, not a test of the board you are buying or allowable structural design values. Grain, defects, moisture, dimensions, joints, and treatment can change the result. An asterisk beside Janka marks an estimate; open the species page for its source and method. Use the header settings to switch units.
Frequently asked questions
Does the hardest wood make the best deck?
Hardness helps with dents but can increase machining time and fastener demands. A softer, correctly treated and installed product may fit a particular budget and maintenance plan better.
Will deck boards keep their original color?
Sun and weather usually change exposed wood's color. Retaining a fresh appearance requires a compatible maintenance system; durability and color retention are separate goals.
What should I inspect on an existing wood deck?
Look at persistent wet areas, board ends, fasteners, edges, and places where furniture or planters obstruct drying. Check for loose boards, splinters, and visible deterioration. A sound-looking walking surface does not establish the condition of the frame beneath it, so assess the supporting structure separately when deciding what needs repair.
Sources and further reading
The application advice is editorial guidance. The references below provide background; each wood's measured values have their own sources on its species page.
- USDA Forest Products Laboratory — Wood Handbook
Background on wood properties, moisture, construction, and finishing.