Batai vs Kokko

Albizia falcataria against Albizia lebbek. Every number below names the publication it came from.

PropertyBataiKokko
Janka hardness344 lbfEstimateUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-11a1,240 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC24.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)39.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture8,400 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)—
Modulus of elasticity1.28 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)—
Crushing strength4,490 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)—
Volumetric shrinkage(lower is better)9.5%Chudnoff 1984, Tropical Timbers of the World (AH-607)9.6%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.94Chudnoff 1984, Tropical Timbers of the World (AH-607)2.00Chudnoff 1984, Tropical Timbers of the World (AH-607)

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-11apublic domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.