Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Fava-orelha-de-negro vs Canalete

Enterolobium schomburgkii against Cordia spp. (hard-wooded, dark-colored Gerascanthus group). Every number below names the publication it came from.

PropertyFava-orelha-de-negroCanalete
Janka hardness2,346 lbfLPF/SFB Madeiras Brasileiras2,200 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)58.2 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture23,440 lb/in²LPF/SFB Madeiras Brasileiras—
Modulus of elasticity2.43 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras—
Crushing strength11,407 lb/in²LPF/SFB Madeiras Brasileiras—
Volumetric shrinkage(lower is better)12.7%LPF/SFB Madeiras Brasileiras11.6%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)2.21LPF/SFB Madeiras Brasileiras1.85Chudnoff 1984, Tropical Timbers of the World (AH-607)

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.