Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Faveira vs Faveira

Parkia multijuga against Parkia nitida = Parkia oppositifolia. Every number below names the publication it came from.

PropertyFaveiraFaveira
Janka hardness668 lbfLPF/SFB Madeiras Brasileiras621 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC28.2 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-927.5 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture8,791 lb/in²LPF/SFB Madeiras Brasileiras8,100 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity1.25 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras1.19 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength5,362 lb/in²LPF/SFB Madeiras Brasileiras4,693 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)9.8%LPF/SFB Madeiras Brasileiras7.9%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)2.41LPF/SFB Madeiras Brasileiras2.00LPF/SFB Madeiras Brasileiras

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons

Published comparisons

400 selected pairs, each with a published Janka test for both woods.