Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Hoop-Pine vs Parana-pine

Araucaria spp. against Araucaria augustifolia. Every number below names the publication it came from.

PropertyHoop-PineParana-pine
Janka hardness576 lbfEstimateUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-11a780 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC31.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)34.7 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture11,000 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)13,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity1.56 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.61 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength5,840 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)7,660 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)—11.6%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)—1.98USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-11apublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons

Published comparisons

400 selected pairs, each with a published Janka test for both woods.