Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Kapur vs Keruing

Dryobalanops spp. against Dipterocarpus spp.. Every number below names the publication it came from.

PropertyKapurKeruing
Janka hardness1,230 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b1,270 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC49.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-954.2 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture18,300 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b19,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity1.88 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.07 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength10,090 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b10,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)14.8%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-416.1%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)2.22USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-42.10USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons

Published comparisons

400 selected pairs, each with a published Janka test for both woods.