Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Oak vs Cherrybark oak

Quercus spp. against Quercus pagoda. Every number below names the publication it came from.

PropertyOakCherrybark oak
Janka hardness2,500 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b1,480 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Density at 12% MC53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)47.6 lb/ft³USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Modulus of rupture23,000 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b18,100 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Modulus of elasticity3.02 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.28 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Crushing strength2,960 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)8,740 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Volumetric shrinkage(lower is better)18.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4—
Tangential / radial ratio(lower is better)1.83USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4—

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3bpublic domain
  • USDA FIA REF_SPECIESpublic domain
  • GWDD v2.2 (Fischer et al. 2026)CC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons

Published comparisons

400 selected pairs, each with a published Janka test for both woods.