PropertyTotaraPodocarp
Janka hardness655 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)760 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC32.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)35.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture9,360 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)11,800 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity1.38 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.38 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength5,850 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)6,980 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)10.4%Chudnoff 1984, Tropical Timbers of the World (AH-607)9.6%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.73Chudnoff 1984, Tropical Timbers of the World (AH-607)2.46Chudnoff 1984, Tropical Timbers of the World (AH-607)

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.