Wood Record

Compare two woods

Choose any two species to compare their published properties. Search by common or scientific name. Your selections stay in the URL, ready to share.

Eastern hemlock vs Western hemlock

Tsuga canadensis against Tsuga heterophylla. Every number below names the publication it came from.

PropertyEastern hemlockWestern hemlock
Janka hardness500 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b540 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Density at 12% MC28.0 lb/ft³USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b31.5 lb/ft³USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Modulus of rupture8,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b11,300 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Modulus of elasticity1.20 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b1.63 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Crushing strength5,410 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b7,200 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Volumetric shrinkage(lower is better)9.7%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-312.4%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Tangential / radial ratio(lower is better)2.27USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-31.86USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3public domain
  • USDA FIA REF_SPECIESpublic domain
  • GWDD v2.2 (Fischer et al. 2026)CC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons

Published comparisons

400 selected pairs, each with a published Janka test for both woods.